Guides / Application guide
Film Thickness Measurement: Wet and Dry (WFT/DFT)
How to measure wet and dry film thickness: gauge types, how many readings to take, the WFT-to-DFT formula with a worked example, and out-of-range fixes.
Why film thickness matters
Every coating has a target dry film thickness (DFT) range, printed on its technical data sheet (TDS). Applying within it matters as much as surface preparation. Outside it, failures are predictable:
| Failure type | Cause | Result |
|---|---|---|
| Pinhole rusting | DFT too low — substrate profile peaks through the film | Localised electrochemical corrosion at exposed peaks |
| Britling | Primer applied below target DFT | Poor intercoat adhesion; topcoat flexibility lost |
| Sagging / running | DFT too high — viscosity and gravity conflict | Inconsistent film, uneven protection |
| Stress cracking | Epoxy applied above target DFT | Residual stress exceeds adhesion strength — cohesive fracture |
| Wrinkling | Alkyd topcoat too thick | Topcoat skins before undercoat — relative motion causes surface distortion |
A 0.5mm variance in wet film thickness can change the final DFT by 32–50% of the target value.
Measuring wet film thickness (WFT)
Measure WFT immediately after application, before any drying occurs. Wet film gauges (ISO 2808, ASTM D4414) are the only check you can still act on: if the reading is low, add paint while it is wet.
| Tool | Tolerance | Method |
|---|---|---|
| Comb gauge | ±5% | Press into wet film; highest notch that contacts the film indicates WFT |
| Wheel gauge | ±2.5% (+1μm) | Roll across wet film; eccentric edge marks WFT at touch-dry point |
Notes:
- Clean gauges with solvent immediately after each reading
- Wheel gauge: inspect eccentric surface for chips before use — chips cause skip marks and inaccurate readings
- Apply at 3 or more random points per panel/area to capture thickness variation
Measuring dry film thickness (DFT)
Measure DFT once the coating has cured, with a gauge that suits the metal underneath. Magnetic and electronic gauges are non-destructive: they read through the paint to the metal.
| Gauge | Substrate | How it works |
|---|---|---|
| Magnetic pull-off gauge | Steel and iron | A magnet is pulled off the surface; the thicker the film, the less force it takes. No batteries, but slower and less precise. |
| Electronic gauge, magnetic induction | Steel and iron | A probe measures the gap to the steel. Fast, and most models store readings and averages. |
| Electronic gauge, eddy current | Aluminium and other non-ferrous metals | A probe senses the metal through the film. Dual gauges switch between the two methods automatically. |
| Destructive (paint inspection gauge) | Any | Cuts a small V-groove and shows each coat under a magnifier. Use only when you need coat-by-coat thickness; repair the cut. |
On galvanised steel, a magnetic gauge reads the zinc and the paint together. Measure the zinc before painting, or subtract it afterwards.
Calibrate and check the gauge
- Check the gauge against certified shims or standards at the start and end of each session, at a thickness close to the one you expect.
- On blasted steel the gauge reads slightly high, because the probe sits on the peaks of the profile. Take a base reading on bare blasted steel (SSPC-PA 2) or use the correction value in ISO 19840, and subtract it.
- Record the mean and range; both minimum and maximum readings matter.
How many readings to take
Film thickness varies across every surface, so one reading tells you little. Inspection standards set both a sampling plan and a pass rule. The two in common use are below; as general practice, follow whichever your specification names.
- ISO 19840: the number of readings rises with the area, from 5 for an area up to 1 m², to 30 for 30–100 m², plus 10 for each further 100 m². The area passes if the average is at or above the nominal DFT, no reading is below 80% of it, and no more than 20% of readings fall between 80% and 100%.
- SSPC-PA 2: a spot measurement is the average of at least three readings within a 4 cm (1.5 inch) circle. Take five spots in each 10 m² (100 ft²) area. By default a single spot may fall to 80% of the minimum or reach 120% of the maximum, but the average of the five must be within the specified range.
- Add readings at edges, welds, bolts and corners. Films are thinnest there, and that is where rust starts.
WFT to DFT calculation
Paint shrinks as the solvent evaporates. What stays on the surface depends on the volume solids: the share of the wet paint, by volume, that remains as dry film. It is also called non-volatile content (NVC) by volume, and the TDS gives it.
DFT = WFT × volume solids % ÷ 100
To work backwards from a target: WFT = DFT ÷ (volume solids % ÷ 100)
Worked example: road marking paint has ± 46% volume solids and a target of 150 µm DFT on a new road, both from its TDS. The wet film to apply is 150 ÷ 0.46 ≈ 326 µm. A re-coat at 75 µm DFT needs about 163 µm wet.
The same sum explains the WFT ranges printed on some datasheets. FPW15 primer is ± 15% solids, so its 20–35 µm DFT range becomes 130–230 µm WFT on its TDS.
Thinning raises the WFT you need, because thinner adds volume but no solids. A paint at 40% volume solids thinned by 10% falls to about 36% (40 ÷ 1.10), and 50 µm DFT then needs about 138 µm wet instead of 125 µm. Thin only with the thinner and amount the TDS allows.
If a TDS gives solids without saying "by volume", treat the result as an estimate and confirm it with a dry film gauge.
If film thickness is out of range
| Situation | Action |
|---|---|
| DFT below minimum | Apply an additional coat once the existing film has cured to the minimum recoat window |
| DFT above maximum | Do not apply additional coats; allow full cure; consult TDS or contact Marindec technical support |
For product-specific DFT ranges, recoat windows, and dilution rates, refer to the Technical Data Sheet (TDS) for each Marindec product.