The rule
A surface must be clean and sound before any primer goes on. Paint applied over oil or dust bonds to the contaminant, not the metal, and lifts off with it.
Steel and iron
Remove millscale (the dark scale left from rolling), rust, oil, grease and dust. Choose the method by how dirty the steel is:
| Method | Removes | Notes |
|---|---|---|
| Solvent cleaning | Oil, grease | Xylene, lacquer thinner or an industrial solvent cleaner. Wipe with a clean lint-free cloth and let it dry. |
| Grit blasting | Millscale, rust | The most effective method. It also roughens the surface so paint can grip. Remove blast dust straight away. |
| Mechanical cleaning | Loose scale, particles | Wire brushing, grinding, vacuuming or air-blowing. |
| Burn-off | Heavy oil and organics | Heat to about 400 °C, then clean mechanically to remove the residue. |
| Where the steel will be | Minimum preparation |
|---|---|
| Industrial or outdoors | Solvent clean, then grit blast to Sa 2½ (near-white metal) |
| Indoors | Solvent clean, then mechanical scrub |
Galvanised steel
The zinc coating forms white rust when exposed to air, and it must come off before painting.
- Clean with galvanised iron cleaner or sugar soap solution.
- Rinse thoroughly with water.
- Let it dry completely.
Weathered galvanised steel has a chalky layer: sand it lightly first, then clean as above. Prime with GI Primer, never red oxide. The full system is in how to paint galvanised steel.
Aluminium
Aluminium forms a thin, invisible oxide layer that paint won't grip.
- Solvent clean to remove oil.
- Sand lightly with fine abrasive paper to break the oxide layer.
- Prime soon after; don't leave it bare for long.
Prime with an etch primer such as EPS15, never red oxide.
Concrete and masonry
- Brush off efflorescence (white salt deposits); acid wash if it is heavy.
- Fill blow holes and cracks, and let the filler cure.
- Let new concrete cure for at least 28 days.
- Check it is dry: tape a plastic sheet to it for 24 hours. Condensation underneath means it is still too damp.
Previously painted surfaces
- Scrape or wire-brush off loose and flaking paint, in spots only unless the whole coating has failed.
- Sand the edges of the remaining paint smooth.
- Wash the whole surface with sugar soap or detergent, rinse and let it dry.
- Prime any bare metal before the topcoat.
On the day
- Paint only when the steel is at least 3 °C above the dew point; below that, moisture condenses on it.
- Prime blasted or wire-brushed steel the same day, before flash rust forms.
Products: Armourphos Cleaner, Paint Remover and Standard Lacquer Thinner. The full method is in our surface preparation guide.