Why this comes first
Most coating failures come from poor surface preparation and application, not the paint. The usual causes are contamination left on the surface, the wrong primer for the material, and the wrong film thickness. Knowing what you are painting avoids the first two.
1. Identify the surface
| Type | Surface | Usually contaminated with |
|---|---|---|
| Ferrous metals (contain iron) | Cast iron | Sand, mould release agents, iron oxide |
| Hot-rolled mild steel | Millscale, iron oxide | |
| Cold-rolled mild steel | Tooling oils, grease, finger marks | |
| Stainless steel | A thin oxide layer | |
| Non-ferrous metals | Galvanised steel | Grease, white rust |
| Aluminium | An invisible aluminium oxide layer | |
| Copper and brass | Surface oxides | |
| Other | Concrete and plaster | Dust, damp, efflorescence (salt deposits) |
| Previously painted | Loose paint, salts, rust, oil |
2. Check what is on it
- Cloth rub: wipe with a clean white cloth. Black residue is millscale, orange or brown is rust, clear or oily is grease.
- Tape pull: press tape on firmly, peel it off and look at what comes away.
- Knife probe: scrape lightly to find loose scale or a soft layer underneath.
3. Do the water spread test
Put a few drops of water on the untreated surface and watch how far they spread. The less they spread, the more contaminated the surface.
| Rating | What the water does | Coating to use |
|---|---|---|
| 1 | Beads up immediately | Solvent-based (heavy contamination) |
| 2 | Spreads poorly | Solvent-based |
| 3 | Spreads moderately | Solvent-based |
| 4 | Spreads well | Water-based is suitable |
| 5 | Spreads fully | Water-based is suitable |
Bare mild steel, aluminium and galvanised steel usually rate 2, and previously painted surfaces 1–2, so they need solvent-based coatings. Bare wood usually rates 5.
4. Clean, then prime
Remove oil and grease with a solvent and loose rust or scale mechanically. See how to prepare steel, galvanised iron and aluminium. Then choose the primer:
| Surface | Primer |
|---|---|
| Mild and structural steel | FPW15 Red Oxide Primer |
| Aluminium | EPS15 Etch Primer |
| Galvanised steel and IBR (inverted box rib) roof sheeting | GI Primer |
Red oxide primer for steel cannot be used on galvanised steel or aluminium. The full method is in our surface examination guide.