Why thickness matters
Every coating has a target dry film thickness (DFT): the thickness of paint left on the surface once it has cured, measured in microns (µm). The range is printed on the product's technical data sheet (TDS). Outside that range, failures are predictable:
| Problem | Cause | What you see |
|---|---|---|
| Pinhole rusting | Film too thin: the peaks of the steel's surface profile poke through | Spots of rust through the paint |
| Brittle primer | Primer below its target thickness | Topcoat doesn't hold and loses flexibility |
| Sagging and runs | Film too thick for the paint to hold on a vertical surface | Uneven film and uneven protection |
| Stress cracking | Epoxy applied too thick | Cracks through the coating |
| Wrinkling | Alkyd topcoat too thick: the surface skins before the coat beneath has cured | A wrinkled, distorted finish |
1. Measure the wet film while you paint
Wet film thickness (WFT) is the thickness of paint just after it goes on. It is the only reading you can still correct, so take it straight away, before the paint starts to dry.
| Gauge | Accuracy | How to use it |
|---|---|---|
| Comb gauge | ±5% | Press it into the wet film. The last notch with paint on it is the reading. |
| Wheel gauge | ±2.5% | Roll it across the wet film. The point where paint marks the wheel is the reading. |
- Take at least 3 readings at random points on each panel.
- Clean the gauge with solvent after every reading.
- Check a wheel gauge for chips before use; a chipped edge gives false readings.
2. Work out the dry thickness
Paint shrinks as the solvent evaporates. What is left depends on the solids by volume (also called non-volatile content), given on the TDS:
Dry thickness = wet thickness × solids % ÷ 100
For example, a paint with 50% solids applied at 100 µm wet leaves about 50 µm dry. To hit a target, work backwards: wet thickness to apply = target dry thickness ÷ (solids % ÷ 100). A 60 µm target at 50% solids means applying 120 µm wet.
Real example: FPW15 Red Oxide Primer is about 15% solids, so its TDS range of 20–35 µm dry means applying 130–230 µm wet.
3. Check the dry film once it has cured
- Use an electromagnetic gauge (an Elcometer or similar) on steel and iron, after full cure.
- Calibrate it against the maker's shims at the start and end of each session.
- Take at least 3 readings at random points on each surface.
- Record the average and the range. The thinnest and thickest readings matter as much as the average.
4. Fix readings that are out of range
| Reading | What to do |
|---|---|
| Below the minimum | Apply another coat once the existing film has cured to its minimum recoat time (on the TDS). |
| Above the maximum | Don't add another coat. Let it cure fully, then check the TDS or contact us. |
Gauge types, how many readings to take and a worked example are in our film thickness measurement guide.